20CrMnTi alloy structural steel wire rod used in our clamp production
1. Raw material – 20CrMnTi wire rod
This is the 20CrMnTi alloy structural steel wire rod used in our clamp production.
We maintain an inventory of approximately 500 tons of raw materials year-round, which can meet the production needs of no less than 2 million clamps per month.
After each batch of raw materials arrives at the factory, it first undergoes incoming material inspection, including testing of outer diameter, surface condition, and chemical composition. Only after confirming that the material meets our technical requirements will it proceed to the next production process.
2. Annealing
After passing inspection, the wire rods first enter the annealing process. Annealing is performed at 760 ℃
using a temperature-controlled annealing machine , held at that temperature for 48 hours, with the temperature difference within the furnace controlled within ±2℃ . This process makes the internal structure of the material more uniform, while reducing hardness and increasing plasticity, preparing it for subsequent cold drawing and cold forming.
We currently have 6 annealing machines, each furnace can process 24 tons, with a daily capacity of approximately 72 tons, which can meet the factory's continuous production needs.
3. Pickling
After annealing, the wire rods enter the pickling process.
The surface of the wire rods is treated with hydrochloric acid solution to remove oxide scale, rust, and other surface impurities formed during annealing and storage, providing a clean surface condition for subsequent phosphating and cold drawing.
The pickling time and solution concentration are strictly controlled according to the surface condition of the material to avoid insufficient or excessive pickling.
4. Phosphating
After pickling, the wire rod enters the phosphating process.
After being treated in the phosphating solution for a specified time, a uniform phosphate conversion film forms on the surface.
This phosphate film improves the adhesion of the lubricant and reduces friction between the steel and the die during subsequent cold drawing, thereby improving cold drawing quality and reducing die wear.
The phosphating time is controlled at 10-15 minutes/hour, after which the wire rod proceeds to the next cold drawing process.
5. Cold Drawing
After surface treatment, the wire rod begins cold drawing.
Using a cold drawing die, the raw material is gradually drawn to the required specification for production.
Cold drawing not only obtains accurate and stable material dimensions but also improves the surface quality, providing a stable blank for subsequent cold forming of the clamping sheet.
After cold drawing, we will inspect the material diameter and surface condition again. Only after confirming that it meets the requirements will it proceed to the cold forming process.
6. Cold Forming
After cold drawing, the material enters the cold forming process for the clamping pieces.
Using automated cold forming equipment, feeding, cutting, and blank forming are continuously completed in the mold, processing the steel into the basic blanks for the clamping pieces.
Compared to traditional machining methods, cold forming maintains the material's fiber flow lines and features high production efficiency, good dimensional consistency, and high material utilization.
We currently have 6 cold forming equipment, with a daily capacity of 240 thousand pieces, providing a stable supply of blanks for subsequent clamping piece processing.
In addition to our own use, we also sell cold-formed blanks to external customers.